ulge in the plate, and to in this article. It had been over- having been put into the testing ma- heated directly over the fire box, mak- chine without straightening. " Burr ing the shell plates wavy. After care- tests" were also made. One of them, fully drawing the water from the boiler heated… … FIGS. 4: plunged in cold water and hammered The conclusions the writer arrives at are, that the importance of mechanical, as shown, without failure. The analy- sis of the ruptured plate is as follows : physical and chemical tests cannot be overrated. While the plate makers Phosphorus 063 per cent.…